Slag inclusion in sand casting is a defect in which slag, the layer of non-metallic oxides that forms on molten metal, is carried into the mold or forms there during filling and ends up trapped on or in the casting. It belongs to the inclusion family of casting defects, alongside sand inclusion.
Welding has a defect with the same name, flux residue trapped between weld beads, and it is unrelated to the casting defect.
What Causes Slag Inclusion
Slag reaches a sand casting by two routes: it is carried over from the furnace or ladle with the pouring stream, or it forms inside the mold when the metal oxidizes during filling.
Slag is a mix of oxides, mostly silica with lime, alumina, manganese oxide and iron oxide. It comes from impurities in the charge, from oxidation of the metal during melting, and from fluxes the melter adds on purpose.
Carried-over slag gets in when the slag cover is not fully skimmed, or when the ladle pours from the top of the bath and slag goes down the sprue with the stream. Slag made in the mold comes from turbulence: metal that drops or jets into the cavity mixes with air and oxidizes as it fills. Ductile iron adds a third source, the dross from its magnesium treatment.
Foundries stop slag in the ladle, in the gating and in the way the metal is poured:
- Skim before pouring: deslag the furnace and ladle, use a flux to separate slag from the metal, and pour from a teapot-spout ladle, which draws metal from below the slag layer.
- Keep the pouring basin full: a full basin keeps floating slag from being drawn down the sprue.
- Pour hot and fast: raise the pouring temperature and shorten the pour, since slag forms faster in cooler metal and with longer exposure. The common advice to pour cooler is a remedy for sand expansion defects.
- Trap slag in the gating: chokes, slag traps and filters hold slag back, and a dead runner extended past the gates collects the first and dirtiest metal.
- Fill without turbulence: a gating system that keeps the stream from dropping or jetting into the cavity stops slag forming in the mold, which matters most in steel and in aluminum and magnesium alloys.
How to Identify Slag Inclusion
Slag inclusion is identified first by where it sits and how it looks: irregular, rough pockets on the upper faces of the casting, often with gas holes beside them. Those clues point to slag, but proof takes a metallographic section through the defect and an analysis of its composition by SEM-EDX (energy-dispersive X-ray analysis in a scanning electron microscope).
Radiography does not settle the question. ASTM E446, a reference-radiograph standard for steel castings, grades sand and slag inclusions together as Category B, so a film graded against it reports an inclusion’s severity without telling slag from sand.
What It Looks Like and Where It Appears
Slag inclusion is mostly a surface defect: slag floats on the metal and collects on the cope faces of the casting, on the undersides of cores and on protruding mold sections. Slag too viscous to rise can freeze in place, so the defect is sometimes internal.
After shot blasting, slag at the surface leaves an irregular, crater-shaped cavity, and slag pockets also show on machined faces. Its appearance varies with the slag it came from, and color is not a dependable way to recognize it.
In iron, a blowhole with slag in or beside it is part of the slag defect rather than a separate gas problem.
Slag Inclusion vs Sand Inclusion
The difference is where the material came from: slag inclusion is oxide from the melt, while sand inclusion is mold or core sand that the flowing metal eroded or that was abraded loose as the mold was closed.
Location is the first clue. Sand inclusion sits where the metal scours the mold face, mostly near the gate and along edges, and often leaves a metal bump on the casting where the sand was washed out of the mold wall. Slag inclusion sits on the upper faces and under cores, where floating material ends up.
The two often appear in the same defect: a sectioned slag pocket may contain sand dissolved from the mold wall, and sand inclusions often carry slag and oxides with them.
Slag Inclusion vs Dross
Dross is one kind of slag, the one made by magnesium treatment in ductile iron and the main form slag takes in aluminum and magnesium alloys, rather than another name for slag inclusion in general.
In ductile iron, dross sits on the casting surface or just under the skin, often with gas bubbles, and because it tends to lie there in thin layers it is also called slag skin.
The word is also used more loosely. In ductile iron, black stains on a fracture face from sand, slag or undissolved inoculant are sometimes classed as dross too.