Gray iron fits a pump casing on clean water at ordinary pressure; higher pressure, freezing, abrasive slurry and corrosive liquids each need a different iron, listed here with the ASTM specification to call on the drawing.
| Duty | Casing iron | ASTM specification |
|---|---|---|
| Clean water, HVAC, irrigation | Gray iron | A48; A278 for pressure-containing parts |
| Higher pressure and surges | Ductile iron | A536; A395 for pressure-retaining parts |
| Freezing and thermal shock | Ductile iron | A536 |
| Abrasive slurry | High-chromium white iron | A532 Class III Type A |
| Corrosive liquids | Ni-Resist or high-silicon iron | A436 or A439; A518 |
Past these duties cast iron stops being the answer. Hazardous liquids and refinery pumps go to cast steel or stainless, and brine circulation pumps have moved their casings to duplex stainless.
Clean Water, HVAC and Irrigation: Gray Iron
A clean-water casing is gray iron to ASTM A48, or to ASTM A278 when the drawing treats it as a pressure-containing part, and it is good to 450 °F under A278 and to 175 psig on the makers’ ratings for 125-class flanges.
Under ASTM A278, gray iron castings of every class are suitable up to 450 °F, and only Class 40 and higher are suitable from 450 °F to 650 °F. The 250 °F limit quoted on some vendor pages is not in the standard.
On a real pump the pressure rating falls with temperature well before the iron reaches those limits. Armstrong’s Series 4300 vertical in-line pump with a cast iron casing and 125-class flanges is rated 175 psig at 140 °F and 100 psig at 300 °F.
For the class, one owner specification, Los Alamos National Laboratory’s for packaged sewage lift stations, calls for ASTM A48 Class 30 on the casing. Calling gray iron to A278 instead of A48 on a pressure casing brings those temperature limits and A278’s stress-relief requirement into the order.
Higher Pressure and Pressure Surges: Ductile Iron
Move the casing to ductile iron when the pump needs a higher rating than a 125-class cast iron casing carries; on named pumps the change comes with 250-class flanges. Armstrong’s end-suction pump specification puts it plainly: a cast iron casing for 175 psig at 140 °F, ductile iron for pressures to 250 psig.
These are each maker’s ratings for its own pumps.
ASTM A536 is the general ductile iron specification. ASTM A395 covers ferritic ductile iron for pressure-retaining parts and names pumps among them: all grades suit service to 450 °F, and only Grade 60-40-18 suits 450 °F to 650 °F. Which A536 grade the casing needs is a separate grade decision.
Freezing and Thermal Shock: Ductile Iron
A casing that may freeze full of water, or take a sudden temperature change, needs ductile iron because ductile iron stretches where gray iron cracks.
Abrasive Slurry and Solids: High-Chrome White Iron
A slurry pump casing is cast in ASTM A532 high-chromium white iron, and Class III Type A, with 23–28% chromium, is specified for both the casing and the impeller of oil-sands tailings pumps.
Class II covers the chromium-molybdenum irons with 11–23% chromium; Class III is used where the slurry also brings some corrosion. A532 orders hardness by delivery condition (as-cast, hardened, stress-relieved or softened for machining), and a tabulation of the standard puts its high-chromium types at 400–600 HB.
The European equivalent is EN 12513, whose highest chromium range runs from 23% to 30% and whose grades are designated by Brinell hardness.
Corrosive Liquids
For a corrosive liquid the casing changes from plain gray or ductile iron to an austenitic Ni-Resist iron (ASTM A436 or A439), to high-silicon iron (ASTM A518), or to a ductile iron casing with a liner.
When Plain Gray or Ductile Iron Corrodes Too Fast
No standard or published study gives a pH, chloride or oxygen level at which a plain iron casing stops being suitable; the “pH 6 to 9” window on vendor pages has no source behind it. In water, check dissolved oxygen first: in a study of ductile iron in simulated pipeline water, it had the largest effect on corrosion, ahead of temperature, immersion time, water hardness, pH and chloride.
Alkaline liquids are no safer for plain iron. In a 2022 study, ductile iron cut from a submersible pump rotor corroded at 1,743 µm/year in aerated synthetic wastewater at pH 11, faster than at pH 3.
A bronze or stainless impeller in a cast iron casing makes the casing the less noble metal of the pair, so in a conductive liquid the casing corrodes faster than it would around an iron impeller.
Ni-Resist and High-Silicon Iron
Ni-Resist is the cast iron for brine and seawater casings, and high-silicon iron fits acid service.
Ni-Resist is iron with enough alloy to make its matrix austenitic: ASTM A436 is the flake-graphite form, ASTM A439 the spheroidal-graphite form. The ductile Ni-Resist grades used for seawater brine pumps, such as A439 D2, carry 18–22% nickel.
High-silicon iron carries 11.5–18.0% silicon. High-silicon iron with 14.5% silicon resists 30% sulfuric acid, and with 16.5% silicon it resists sulfuric and nitric acid at any concentration. ASTM A518 has three grades chosen by the service, with Grade 2 suited to strong chloride environments.
High-silicon iron is brittle and low in mechanical properties, so it suits a casing kept free of shock and heavy piping loads. It also resists alkalis poorly, which keeps it on acid duty.
Lined Ductile Iron Casings
A lined ductile iron casing is used when the liquid would attack or wear any unlined iron and an alloy iron casing would be too brittle or too costly at that size. The rubber or polymer liner’s own temperature and chemical limits then become the casing’s limits.
When the Duty Rules Out Cast Iron
Cast iron is ruled out wherever a cracked casing would release a hazardous or flammable liquid; those pumps go to cast steel, stainless or duplex.
For API 610 pumps, the Hydraulic Institute says cast iron is avoided because of the danger of failure from external shock.
Cast steel is the minimum for a hazardous-liquid pump: cast iron should not be used for hazardous liquids, at pressures above 200 psig or temperatures above 175 °C. Ductile iron should be avoided wherever there is any risk of fire.
Cast iron is also out of long-life brine service: brine circulation pump pressure casings have moved from ductile Ni-Resist to more resistant materials, duplex stainless among them.
Potable Water Service
A drinking-water pump needs certification to NSF/ANSI/CAN 61, which sets health-effects requirements for every material that touches the water. Water pumps can be certified under its Section 8, mechanical devices, and coatings and linings are within the standard’s scope, so a coated casing is evaluated with its coating.
The standard does not prefer ductile over gray iron, so the iron is chosen by pressure and temperature exactly as for any clean-water casing.
Do Coatings Change Which Iron You Need?
No. A coating slows attack on an iron the duty already allows, but it does not qualify a lower iron for a harsher duty.
A full liner designed as the wetted surface is a different case. That is the lined ductile iron casing, where the liner is part of the material choice from the start.