What Are the Allowances Considered for Pattern Making

A pattern carries five allowances: shrinkage, machining, draft, distortion and rapping (also called shake). Each one moves the pattern away from the finished part’s dimensions, so that the casting lands on the drawing after it has cooled and been machined.

Shrinkage, machining stock and draft all make the pattern larger, and distortion reshapes it. Rapping is the only negative allowance: it makes the pattern slightly smaller. How large each one is depends on the metal, the molding method, the size of the casting and how rigid the mold is.

Two of the five belong on your drawing. The machining allowance is called out in a general note, and draft is set in a drawing note agreed with the foundry. The shrinkage allowance, along with any distortion or rapping correction, is the foundry’s own: it depends on that foundry’s sand and process, and it is built into the pattern without appearing on the drawing.

Shrinkage Allowance

The pattern is made larger than the casting by the amount the solid metal contracts as it cools from its freezing temperature to room temperature, stated as a percentage of the casting dimension:

Pattern allowance (%) = (pattern dimension − casting dimension) ÷ casting dimension × 100

The pattern corrects only that solid contraction. The liquid and solidification shrinkage that comes before it does not change the outside size; it shows up as pipe and internal voids, and the gates and risers have to feed it.

The patternmaker applies the allowance with a shrink rule, a scale whose graduations are lengthened by the metal’s allowance, so no arithmetic is needed at the bench.

Shrinkage Allowance by Metal

Steel needs about twice the shrinkage allowance of gray iron, and high-alloy steels need more again. The table gives the general rule-of-thumb values; the high-alloy row covers the austenitic cast stainless grades, while the martensitic and ferritic grades take the carbon steel figure.

MetalShrink rule (in/ft)Allowance (%)
Gray iron1/81.04
Carbon and low-alloy steel1/42.08
High-alloy steel5/162.60

Treat each figure as a starting point. In SFSA’s production measurements, low-alloy steel averaged 1.60% in green sand and 2.39% in no-bake, a wider gap than the one between carbon steel and high-alloy steel in the table.

We do not use a book figure for ductile iron. Its allowance depends on how rigid the mold is, so we set it from our own measured castings on the line the part will run on.

Dimensions held by cores often shrink less than free outer dimensions, though in green sand the difference can disappear or even reverse.

Double Shrinkage Allowance

A pattern needs a double shrinkage allowance when the pattern itself is cast from a master. A production pattern in aluminum or iron, such as a match plate, is poured from a wood master, and the master must carry two allowances: the casting metal’s shrinkage, and on top of that the shrinkage of the metal the pattern is cast in. A plastic pattern molded from a master works the same way, with the plastic’s shrinkage taking the place of the pattern metal’s.

Machining Allowance

Each machined surface gets a required machining allowance (RMA), chosen from the casting’s largest finished dimension and a grade that follows the molding method. On a machine-molded steel casting 250 to 400 mm long, SFSA’s table for steel castings puts that at 2.5 to 5 mm per surface.

Required machining allowance per surface, steel castings, by largest casting dimension (mm)
100–160 mm
1.5–3 mm
2.2–6 mm
1.1 mm
250–400 mm
2.5–5 mm
3.5–10 mm
1.8 mm
630–1,000 mm
3.5–7 mm
5–14 mm
2.5 mm
1,600–2,500 mm
4.5–9 mm
6–18 mm
3.2 mm
Sand, machine molded (grades F–H)
Sand, hand molded (grades G–K)
Investment (grade E)

The drawing states which surfaces are machined, plus the RMA value and grade, and one value normally applies to every machined surface on the casting. On a diameter, or a feature machined on both sides, the allowance counts twice.

An investment casting needs much less stock. The standard values for steel are conservative for short runs and can come down on high-volume work after machining trials. For gray and ductile iron, the grade is agreed with the foundry.

Cope surfaces of a large casting need more stock than drag surfaces or side walls. Less than 6 mm on a cope face is generally not recommended, so critical machined faces should be molded in the drag where the design allows. On any surface, the stock should let the first cut stay at least 1.5 mm (1/16 in) below the cast skin.

When machining stock and shrinkage apply to the same dimension, add the stock first and apply the shrinkage to the result. A carbon steel part 500 mm long, machined on both ends with 6 mm per end, becomes a 512 mm casting and, at 2.08%, a 522.6 mm pattern; draft is added on top of both.

Draft Allowance

In SFSA’s typical values, steel sand castings take a taper of about 1° to 2° on every surface perpendicular to the parting line, with the most for manual green sand and deep pockets and the least for machine-molded, no-bake and shell molds.

Typical draft (taper) allowance for steel castings by molding process (degrees)
Green sand, manual
1.5 °
2 °
Green sand, automated
1 °
1.5 °
No-bake and shell
1 °
1.5 °
Most features
Deep pockets

Interior surfaces need more draft than exterior ones. The angle also falls as a surface gets taller, although the taper measured in millimetres still grows: ISO 8062-3’s grade A default for a hand-molded external surface drops from 2.2° at 25 to 40 mm high to 1.0° at 100 to 160 mm.

Set draft in a drawing note agreed with the foundry, and where it affects fit, say whether it adds to or subtracts from the drawn dimensions. Unless the drawing says otherwise, ISO 8062-3 adds the taper as extra material.

An investment casting needs a fraction of these angles and sometimes none at all, while a permanent metal mold needs more than sand on surfaces taller than about 16 mm.

Distortion Allowance

A casting that warps as it cools gets a pattern bent the opposite way by the amount it is expected to move, so the casting comes out to shape. In a U-shaped casting, whose legs spread as it cools, the pattern’s legs are made to converge slightly so the cast legs end up parallel.

Most castings need no distortion allowance. It is for uneven contraction the design cannot remove, and open shapes such as a U, an H or a C are the usual cases.

There is no table for the amount; it comes from the foundry’s experience with similar castings or from trial castings. Simulating the stresses during solidification and cooling can predict it instead.

Rapping (Shake) Allowance

A pattern is made slightly smaller for rapping, but the amount cannot be given as a reliable figure. Before drawing the pattern, the molder knocks or jars it loose, which enlarges the cavity a little; the allowance offsets that and applies only to dimensions parallel to the parting plane. If a pattern quote lists a rapping allowance, read it as that shop’s own figure.

Other Allowances Sometimes Listed

Some lists add items that turn out to be another name for one of the five, a pattern feature, an effect already inside the shrinkage figure, or an addition worked out for one job:

  • Finish allowance: the machining allowance under another name, meaning stock left on the casting for machining.
  • Patternmaker’s shrinkage: the trade name for the shrinkage allowance. Lists that describe it as an allowance for wood drying have the term wrong.
  • Core prints: projections on the pattern that locate and anchor the core in the sand. They are a feature of the pattern, listed beside the allowances.
  • Mold wall movement: a real effect, but the pattern carries no separate allowance for it. It is part of the net contraction a casting shows, so the foundry’s measured shrinkage allowance already includes it.
  • Machining lugs and tool clearance: older foundry manuals list lugs for setting the casting up in the machine and clearance for the cutting tool, both worked out for each job.