How to Design a Cast Counterweight for a Tight Envelope

To design a cast counterweight for a tight envelope, divide the required moment by the lever arm and the net volume to get a target density, then choose a material that reaches it. As a rough guide from measured densities, gray iron fits up to about 7.1 g/cm³ and cast steel covers about 7.2 to 7.7 g/cm³. Above that, you need a lead-filled cast shell.

This method assumes the cavity is fixed and the machine sets the moment. With room to spare, density stops being the limit, and the choice moves to grade and casting process.

The target density can still move after you calculate it, because a longer arm lowers it. An arm 5% longer cuts the target density by about 5%, so check Step 3 before you pay for steel.

Step 1: Convert the Envelope and Moment Into a Target Density

Target density is the required moment divided by the arm and the net volume.

Required mass:

m = M / r

Target density:

ρ = M / (r × V)

M is the required moment in kg·m. The arm r is the distance in meters from the pivot to the counterweight’s center of mass, not to its outer face or its bolt line. V is the net volume in liters, and with these units ρ comes out in kg/L, where 1 kg/L = 1 g/cm³.

V must be the net figure: what is left after the tolerance, draft and paint deductions in Step 5, minus the holes and pockets in Step 6. Use an estimate on the first pass, then rerun this calculation with the real figure.

Step 2: Choose a Material That Reaches That Density

The best counterweight material is the cheapest one whose density clears the target. That order runs gray iron, cast steel, then a lead-filled cast shell. The chart shows measured gray iron against steel, lead and the densities calculated for shells holding 20% to 50% lead by volume.

Density at room temperature; shell bands calculated for 20% to 50% lead by volume (g/cm³)
Gray iron, measured
7.11–7.19 g/cm³
Steel
7.8 g/cm³
Gray iron shell with lead
7.99–9.25 g/cm³
Steel shell with lead
8.51–9.57 g/cm³
Lead
11.34 g/cm³

When Gray Iron Fits

Gray iron is enough when the target density is at or below about 7.1 g/cm³. A target of 7.1 to 7.2 g/cm³ depends on the actual iron and needs a checked density or a trim allowance.

Gray iron is often quoted at 7.2 to 7.5 g/cm³, but a 2024 study measured three gray irons at 7.11 to 7.19 g/cm³, one outlier aside.

A stronger iron does not solve a density problem. The strongest iron in that study was only about 1% denser than the weakest.

When to Move to Cast Steel

Move to cast steel when the target density sits between about 7.2 and 7.7 g/cm³ and a longer arm cannot close the gap. Steel is about 7.8 g/cm³, so the 7.7 g/cm³ limit leaves a 1% margin.

When a Lead-Filled Cast Shell Is Needed

A lead-filled cast shell is needed when the target density is above about 7.7 g/cm³ and the arm cannot grow. Lead is 11.34 g/cm³. The share of lead comes from the shell density:

f = (target density − shell density) / (11.34 − shell density)

Here f is lead’s share of the net volume. Use about 7.15 g/cm³ for a gray iron shell and 7.8 g/cm³ for a steel shell on the first pass, then rerun with the density measured in Step 4. The upper limit on f is how much metal the pocket leaves for walls, bolts and lifting points.

One pour does not fill a pocket. Lead loses about 6% of its volume between liquid at its melting point and solid at room temperature, so it stands off the walls unless the pocket holds it.

Plan the lead as a separate job. A ferrous foundry casts the shell and cores the pocket, and melting lead brings whoever fills it under OSHA’s lead standard. Weigh the first filled part to prove the fill.

Step 3: Shape the Casting to Move the Center of Mass

With volume capped, the moment comes from where the metal sits, so put the metal as far from the pivot as the envelope allows. Each piece of the casting counts as its mass times its own distance from the pivot:

x_G = Σ(m_i × x_i) / m_total

Here x_G is the center of mass, m_i is the mass of one piece and x_i is the distance to that piece’s center of mass. Measure every x_i from the pivot, and count a pocket or core as negative mass. In a one-alloy casting the center of mass is the centroid, so the CAD model gives it directly. In a lead-filled shell each piece carries its own density, so put the pocket at the far end.

Take bolt access, clearance cuts and pockets from the pivot side, where each liter costs the least moment. If part of the envelope is still empty, fill the far side first. A solid casting that already fills the cavity has no shape move left, because the cavity sets its arm.

If the machine caps total mass as well as moment, a core near the pivot removes mass at a small cost in moment and moves x_G outward.

Step 4: Account for Shrinkage Porosity in Solid Sections

Account for shrinkage porosity by choosing the material from the low end of its density, then weigh the first castings and divide by the measured volume to get the real figure. Hold a trim allowance when the target is within 1% of the material’s density.

Shrinkage porosity takes mass out of a solid section wherever that section freezes last without feed metal. Steel carries far more of that risk than gray iron. If a thin section lies between a solid block and its feed, it freezes first and cuts the block off. Any padding added to carry feed into the block must fit inside the envelope, so design it in as part of the shape.

Step 5: Stack Casting Tolerance Against the Envelope

Casting tolerance and draft take far more of the envelope than paint. On a 500 mm dimension of a part 300 mm tall, the three add about 2.8 mm to 11.5 mm of cavity width before any running clearance. The 11.5 mm figure is the hand-molded case and the 2.8 mm figure is the machine-molded case with taper in the model:

  • Casting tolerance: Add half the band, because the band sits evenly around nominal. At 500 mm, CT12 is 10 mm total, so it adds 5 mm, and CT10 adds 2.5 mm.
  • Draft: ISO/FDIS 8062-3:2022 lists 3.1 mm of Grade A draft for a hand-molded external face 250 to 400 mm tall. If the taper sits outside the model and both faces widen this dimension, that adds 6.2 mm. If the taper is already in the nominal model, it adds nothing.
  • Paint: A 160 µm alkyd system adds 0.32 mm across two faces, which matters only on machined fits.

The chart gives the total tolerance band for three grades by dimension, from the CT table of ISO 8062:1994. ISO 8062-3 has replaced that edition and renamed the grades DCTG, so check the current table before you fix a value on the drawing.

Total casting tolerance by raw casting dimension, ISO 8062:1994 Table 1 (mm)
Over 160 to 250 mm
4 mm
8 mm
14 mm
Over 250 to 400 mm
4.4 mm
9 mm
16 mm
Over 400 to 630 mm
5 mm
10 mm
18 mm
Over 630 to 1,000 mm
6 mm
11 mm
20 mm
Over 1,000 to 1,600 mm
7 mm
13 mm
23 mm
CT10
CT12
CT14

The grade depends on the molding method. These grades come from the 1984 edition of ISO 8062, so treat them as a starting guide:

Molding methodGray and ductile ironSteel
Machine-molded sand or shell, long seriesCT8 to 10CT8 to 10
Hand-molded sand, long seriesCT11 to 13CT11 to 13
No-bake sand, short seriesCT11 to 13CT12 to 14
Green sand, short seriesCT13 to 15CT13 to 15

Two choices on the drawing save room. First, show the taper in the nominal model, because ISO 8062-3 otherwise applies taper plus, which adds the taper to the tolerance. Second, agree an asymmetric band with the foundry where one dimension is critical. An all-minus band on a CT12 500 mm dimension puts the whole 10 mm below nominal. The largest casting is then 5 mm smaller, though the average casting also loses 5 mm of length.

Do not add parting-line mismatch separately, because it stays within the tolerance band unless the drawing says otherwise. Set the nominal so the largest casting clears the cavity. The smallest casting is one full band smaller, so run Step 1 on that casting’s volume when the required moment is a minimum. If it falls short, tighten the tolerance grade, move the center of mass outward, or go up a material.

Step 6: Fit Mounting Features Inside the Envelope

Machine the mounting faces and the bolt pattern after casting, and take the holes and counterbores out of net volume.

Machining also lets a mounting face sit right at the envelope limit. The raw dimension on a face machined from one side is:

R = F + RMA + CT/2

R is the raw dimension, F the finished dimension and RMA the required machining allowance.

Place the finished face at the limit and leave the as-cast faces at their Step 5 margin. Count mass on the finished shape, since the stock leaves as chips.

Bolt spacing takes up face area. Aerospace joint practice uses a nominal edge distance of 2D from the hole center, a minimum of 1.5D and a spacing of 4D. Use these as starting values, since plate thickness can change them.

A tapped hole also needs depth inside the envelope. Where the full bolt strength is required, size the thread engagement so the bolt breaks before the cast threads strip:

L = 3P / (π × d_m × F_s)

L is the length of thread engagement and P the load at full bolt strength. The mean diameter of the threaded hole is d_m, about the pitch diameter, and F_s is the shear strength of the weaker material. Look up the head height for the bolt you choose and keep the head inside the envelope.

Use dowels to locate the part, and leave them out of the bolt load path.

If the weight has to come off in sections small enough for a shop lift, give each section its own machined faces, bolt pattern and lifting point, and run this step for each one.

Worked Example

These inputs are illustrative and do not come from a real part: a required moment of 300 kg·m, an arm of 1.00 m and a net volume of 40 L after the Step 5 deductions.

  1. Required mass: 300 kg·m / 1.00 m = 300 kg.
  2. Target density: 300 kg / 40 L = 7.50 g/cm³.
  3. Gray iron: 40 L at 7.11 to 7.19 g/cm³ weighs 284 to 288 kg, so at a 1.00 m arm the moment is 284 to 288 kg·m, which is 4 to 5% short.
  4. Cast steel: 40 L at 7.8 g/cm³ weighs 312 kg, so the moment is 312 kg·m, which is 4% over. The 12 kg surplus is trim margin.
  5. Gray iron with a longer arm: Moving the center of mass out 50 mm to 1.05 m drops the required mass to 286 kg and the target density to 7.14 g/cm³.

On these numbers, cast steel passes with margin. Gray iron works only if the same 40 L can sit 50 mm farther out, and 7.14 g/cm³ falls inside the gray iron range with no margin, so it needs a checked density or a trim allowance.

Now tighten the net volume to 34 L at the same moment and arm. The target density rises to 8.82 g/cm³, and 34 L of steel at 7.8 g/cm³ weighs 265 kg, which is 35 kg short, so this case needs a lead-filled shell.

A gray iron shell at 7.15 g/cm³ needs 40% lead by volume. In the 34 L part, the gray iron shell holds 13.6 L of solid lead at 154 kg plus 20.4 L of iron at 146 kg, for a total of 300 kg. A steel shell at 7.8 g/cm³ needs 29% lead by volume, which is 9.8 L of lead at 111 kg. Allow about 6% more liquid lead than the solid volume.